氰化尾渣高温脱氰固硫工艺及机理研究
CSTR:
作者:
作者单位:

1.东北大学 矿物加工科学与技术全国重点实验室,辽宁 沈阳 110819 ;2.东北大学 资源与土木工程学院,辽宁 沈阳 110819

作者简介:

张裕海(1990-),男,山西怀仁人,工程师,研究方向为选冶固废的资源化利用;

通讯作者:

中图分类号:

基金项目:

国家自然科学基金项目(52504285);辽宁省博士科研启动基金计划项目(2025-BS-0123);国家资助博士后研究人员计划项目(GZC20240228);中国博士后基金项目(2025M773606)


Mechanisms of cyanide decomposition and sulfur fixation during high temperature treatment of cyanide tailings
Author:
Affiliation:

1. State Key Laboratory of Mineral Processing, Northeastern University, Shenyang 110819 , China ;2. School of Resources and Civil Engineering, Northeastern University, Shenyang 110819 , China

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    针对氰化尾渣中氰化物难以彻底脱除且易在高温冶炼过程中引发环境风险的问题,本文以山东某金精矿氰化尾渣为研究对象,系统研究了氧化焙烧条件下氰化物的脱除行为及硫化物的迁移转化特征。通过调控焙烧温度、时间、氧气浓度及气体流量,明确了焙烧脱氰的适宜工艺条件,并分析了焙烧过程中硫的固化特性及其对脱氰过程的影响。结果表明,在焙烧温度500℃、焙烧时间30 min、空气气氛及气体流量400 mL·min-1条件下,氰化尾渣中总氰化物脱除率可达97.36%,焙烧产物的毒性浸出液中氰化物浓度降至0.187 mg·L-1,满足国家排放标准要求。研究发现,焙烧过程中碳酸盐矿物分解生成的CaO、MgO及硫化矿氧化形成的铁氧化物可对SO2产生原位捕集,使硫以硫酸盐形式部分固定,硫固化率可稳定保持在60%以上;同时,硫化物氧化释放的SO2在一定条件下与O2协同作用,进一步促进了氰化物的氧化分解。结合XPS表征与热力学分析,阐明了Fe-CN配合物结构破坏及含氰物种彻底去除的机理。研究结果表明,氧化焙烧可在实现氰化尾渣高效脱氰的同时有效降低硫的气相释放负荷,为氰化尾渣在高温协同冶炼体系中的安全配入与污染控制提供了理论依据和技术支撑。

    Abstract:

    Given the difficulty in completely removing cyanide from cyanide tailings and the associated environmental risks during high-temperature smelting, this study investigates cyanide tailings derived from a gold concentrate in Shandong Province and systematically examines cyanide removal behavior as well as the migration and transformation of sulfide minerals under oxidative roasting conditions. By systematically regulating roasting temperature, residence time, oxygen concentration, and gas flow rate, the optimal operating conditions for cyanide removal were identified, and the sulfur fixation behavior and its influence on the cyanide removal process were analyzed. The results indicate that at a roasting temperature of 500°C for 30 min under an air atmosphere with a gas flow rate of 400 mL·min-1, the total cyanide removal efficiency reached 97. 36%, and the cyanide concentration in the leachate of the roasted product decreased to 0. 187 mg·L-1, satisfying national discharge standards. The study demonstrates that CaO and MgO generated from the decomposition of carbonate minerals, together with iron oxides formed by sulfide oxidation, can capture SO2 in situ during roasting, thereby partially fixing sulfur in the form of sulfates, with the sulfur fixation efficiency remaining stably above 60%. Meanwhile, SO2 released from sulfide oxidation can synergistically enhance the oxidation and decomposition of cyanide in the presence of O2 under appropriate conditions. Combined XPS characterization and thermodynamic analysis elucidated the mechanism underlying the breakdown of Fe-CN complexes and the complete elimination of cyanide-containing species. Overall, the results confirm that oxidative roasting enables efficient cyanide removal from tailings while significantly reducing sulfur-bearing gaseous emissions, thereby providing both theoretical insight and technical support for the safe utilization and pollution control of cyanide tailings in high-temperature co-smelting systems.

    参考文献
    相似文献
    引证文献
引用本文

张裕海,赵前飞,赵冰,等. 氰化尾渣高温脱氰固硫工艺及机理研究[J]. 中国有色冶金,2026,55(3):54-66.

复制
分享
相关视频

文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2025-12-18
  • 最后修改日期:
  • 录用日期:
  • 在线发布日期: 2026-07-08
  • 出版日期:
文章二维码