工业钛液碱中和法制备水解晶种稳定性机制研究
CSTR:
作者:
作者单位:

1.攀枝花学院 钒钛学院,四川 攀枝花 617000 ;2.钒钛关键战略材料四川省重点实验室,四川 攀枝花 617000

作者简介:

杜肖阳(2003—),男,四川成都人,硕士研究生在读,主要从事电子级二氧化钛制备等方面的研究。

通讯作者:

中图分类号:

TF823;TF125

基金项目:

四川省科技计划项目(2025ZNSFSC0379,2024ZHCG0141);攀枝花市科技计划项目(25KJJH0025);攀枝花学院研究生创新计划项目(y2025021)


Stability mechanism of hydrolysis seed prepared by alkali neutralization method of industrial titanyl sulfate solution
Author:
Affiliation:

1.School of Vanadium and Titanium, Panzhihua University, Panzhihua 617000 , China ;2.Vanadium and Titanium Critical Strategic Materials Key Laboratory of Sichuan Province, Panzhihua 617000 , China

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    水解晶种稳定性对硫酸法钛白工艺的水解至关重要,本研究以工业硫酸氧钛液为原料,采用碱中和法制备水解晶种,系统分析碱钛比、熟化温度和熟化时间对晶种稳定性的影响机制,并综合运用多尺度表征方法,探究工艺-结构-性能之间的内在关联,得到以下主要结论。碱钛比、熟化温度及熟化时间均通过影响反应进程及体系性质,进而影响工业钛液水解晶种的稳定性,适当增加这些工艺参数值,可以促进晶核的成核速率和生长速率;工业钛液水解晶种的最佳工艺参数为碱钛比 14%、熟化温度 95℃、熟化时间 18~21 min、搅拌速度 300 r/min,在此条件下,晶种稳定性稳定处于 100~130 mL合格区间,水解率为 10.16%,验证实验重复性良好;水解晶种粒径在 21±6.5 nm 范围,粒径分布窄,确保了晶种的高稳定性与活性;优化后晶种的Ti—O键增强、团簇结构致密化,且钛-硫-氧配位结构改善,显著提高表面稳定性。该研究为硫酸法钛白工艺提供了高稳定性晶种制备新策略。

    Abstract:

    The stability of hydrolytic seeds is crucial for the hydrolysis process in the sulfate process for titanium dioxide production. Using industrial titanyl sulfate solution as raw material, hydrolysis seeds were prepared by alkali neutralization method. The effects of alkali-to-TiO2 ratio, aging temperature, and aging time on seed stability were systematically investigated, and the intrinsic relationship between process-structure-performance was explored by using multiple analytical methods, and the following main conclusions were obtained. The alkali-titanium ratio, curing temperature and curing time all affect the stability of the hydrolyzed seed crystal by affecting the reaction process and system properties. Appropriate increase of these process parameters can promote the nucleation rate and growth rate of the crystal nucleus; The optimum process parameters for the hydrolysis of industrial titanium liquid are as follows: alkali-titanium ratio 14%, curing temperature 95℃, curing time 18-21 min, stirring speed 300 r/min. Under these conditions, the stability of seed crystal is stable in the qualified range of 100-130 mL, the hydrolysis rate is 10. 16%, and the repeatability of the verification experiment is good. The particle size of the hydrolyzed seed is in the range of 21±6. 5 nm, and the particle size distribution is narrow, which ensures the high stability and activity of the seed. After optimization, the Ti—O bond of the hydrolysis seed is strengthened, the cluster structure is densified, and the Ti—S—O coordination structure is improved, significantly enhancing surface stability. This study provides a novel strategy for preparing highly stable seeds for titanium dioxide production by the sulfate process.

    参考文献
    相似文献
    引证文献
引用本文

杜肖阳,王青鸿,吴越,等 . 工业钛液碱中和法制备水解晶种稳定性机制研究[J]. 中国有色冶金,2026,55(1): 17-23.