极低品位硫钴精矿钴回收工艺试验
CSTR:
作者:
作者单位:

1.白银有色集团股份有限公司, 甘肃 白银 730900 ; 2.西北矿冶研究院, 甘肃 白银 730900 ;3.中南大学 冶金与环境学院, 湖南 长沙 410083

作者简介:

王栋(1971—),男,甘肃白银人,高级工程师,主要从事科技管理工作。

通讯作者:

中图分类号:

TF816

基金项目:

甘肃省重点研发计划(工业类)湿法炼锌伴生稀有金属钴分离富集新工艺研究(22YF7GD194);甘肃省科技重大专项复杂铅锌矿与多源铅锌固废协同清洁利用关键技术及产业化示范(23ZDGD002)


Experimental study on cobalt recovery process from extremely low-grade cobalt sulfide concentrate
Author:
Affiliation:

1.Baiyin Nonferrous Metals Group Co.,Ltd, Baiyin 730900 , China ;2.Northwest Mining and Metallurgy Research Institute,Baiyin 730900 , China ;3.School of Metallurgy and Environment, Central South University,Changsha 410083 , China

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    随着新能源汽车、储能系统等产业的快速发展,对钴的需求持续增长,钴回收尤为重要。硫钴精矿是将钒钛磁铁矿原矿经过破碎、磨矿、选铁、浮硫等工序加工而得的粉状矿物,主要成分是硫和铁,同时含有贵重金属钴、铜、镍等。硫钴精矿是生产钴产品的主要原料之一,但其中的钴含量通常较低,需要通过进一步的处理和回收来提高其利用价值。本研究针对硫钴精矿的钴品位极低、元素赋存状态复杂的特点,采用氧压浸出工艺。结果表明:控制浸出温度为160±5℃、浸出氧分压1.2MPa、反应时间2h、液固比4∶1、始酸浓度16%的条件下,钴、铜、铁、硫的浸出率分别达到78.5%、75.4%、32.7%、31.4%。硫钴精矿处置直接经济效益为30.36美元/t,按年生产加工80万t硫钴精矿测算,则年毛利润2428.80万美元,具有良好的经济回收前景。

    Abstract:

    With the rapid development of new energy vehicles, energy storage systems and other industries, the demand for cobalt continues to grow, making cobalt recovery particularly important. Sulfur and cobalt concentrate is a powdered mineral obtained by processing raw vanadium and titanium magnetite ore through crushing, grinding, iron beneficiation, sulfur flotation, etc. The main components are sulfur and iron, and it also contains precious metals such as cobalt, copper and nickel. Sulfur cobalt concentrate is one of the main raw materials for the production of cobalt products, but the cobalt content in it is usually low, which needs to be further processed and recovered to improve its utilization value.Thestudy focuses on the characteristics of cobalt sulfide concentrate, which has extremely low cobalt grade and complex element occurrence state. The oxygen pressure leaching process was adopted, and the results show with a leaching temperature controlled at 160±5℃, a leaching oxygen partial pressure of 1.2MPa, a reaction time of 2h, a liquid-solid ratio of 4∶1, and an initial acid concentration of 16%. Under these conditions, the leaching rates of cobalt, copper, iron, and sulfur reach 78.5%, 75.4%, 32.7%, and 31.4%, respectively. The direct economic benefit of disposing of one ton of cobalt sulfide concentrate was $30.36. Calculated based on the annual production and processing of 800000 tons of cobalt sulfide concentrate, the annual gross profit is 24.288 million US dollars, with good economic recovery prospects.

    参考文献
    相似文献
    引证文献
引用本文

王栋,殷勤生,杨斌,等.极低品位硫钴精矿钴回收工艺试验[J].有色设备,2024,38(4):79-85.

复制
分享
相关视频

文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2024-07-13
  • 最后修改日期:
  • 录用日期:
  • 在线发布日期: 2025-11-14
  • 出版日期:
文章二维码