铅烟灰两段混合酸浸工艺回收铟资源的研究
CSTR:
作者:
作者单位:

1.长沙有色冶金设计研究院有限公司, 湖南 长沙 410011 ;2.江西铜业铅锌金属有限公司, 江西 湖口 332500

作者简介:

陈艳梅(1985—),女,陕西榆林人,高级工程师,主要从事有色金属冶炼的咨询与研发工作。

通讯作者:

中图分类号:

TF813;TF843

基金项目:

国家重点研发计划资金资助(2022YFC3901601)


Study on recovery of indium from lead-bearing soot by two-stage mixed acid leaching process
Author:
Affiliation:

1.Changsha Engineering and Research Institute Ltd.of Nonferrous Metallurgy, Changsha 410011 , China ;2.Jiangxi Copper Lead Zinc Metal Co., Ltd., Hukou 332500 , China

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    为解决现行铅烟灰提取铟过程中浸出率低和安全环保问题,提出一种全湿法铅烟灰两段混合酸浸回收铟新工艺。研究铅烟灰浸出过程中硫酸浓度、液固比、反应时间和不同硫酸始酸浓度条件下盐酸对铟浸出率的影响。结果表明,控制铅烟灰一段浸出工艺条件为:液固比8∶1,硫酸始酸浓度150g/L,盐酸始酸浓度40g/L,反应温度90℃,反应时间4h;二段浸出工艺条件为:液固比4∶1,硫酸始酸浓度300g/L,盐酸始酸浓度40g/L,反应温度90℃,铟浸出率达到81.18%,浸出渣含铟0.25%,且产出低酸浸出液符合净化工序要求。铅烟灰两段混合酸浸工艺工业应用后,每年可增产粗铟约3.63t,增加经济效益约553.61万元,该工艺极具推广价值。

    Abstract:

    In order to solve the problems of low leaching rate and safety and environmental protection in the current process of indium extraction from lead-bearing soot, a new process of indium recovery from lead-bearing soot by two-stage mixed acid leaching with full-wet process was proposed.The effects of sulfuric acid concentration, liquid-solid ratio, reaction time and different sulfuric acid initial acid concentration on indium leaching rate during lead-bearing soot leaching were studied.The results indicated that the leaching process conditions were as follows: a liquid-solid ratio of 8∶1, sulfuric acid concentration of 150g/L, hydrochloric acid concentration of40g/L, reaction temperature of 90℃, and a reaction time of 4h. The conditions for the two-stage leaching process were as follows: a liquid-solid ratio of 4∶1, initial sulfuric acid concentration of 300g/L, initial hydrochloric acid concentration of40g/L, reaction temperature at 90℃ with an indium leaching rate at 81.18%, leaching residue containing indium at 0.25%, and low-acid leaching liquid output meeting the purification process requirements. Following the industrial implementation of the lead-soot two-stage mixed acid leaching process, there is a potential increase in crude indium production by approximately 3.63 tons per year and an associated rise in economic benefits by about 5.5361 million yuan, demonstrating significant potential for widespread application.

    参考文献
    相似文献
    引证文献
引用本文

陈艳梅,王峰,王翀.铅烟灰两段混合酸浸工艺回收铟资源的研究[J].有色设备,2024,38(4):44-49.